Transom question
If anyone has redone transom from outside, without reusing outer skin. How many layers of biax 1708 did you use? Did you use mat also?
I am moving along with my repair and want to be sure im on the right track. I've put 6 layers of 1708 on outside now and it seem like i will need some more. I'm learning about fiberglass repair as I go so thanks for any advice. Keith |
Are you pretty much working on it every day over at Hinckley? I'm not doing anything this week and would love to stop by and check it out.
|
Sent you a PM.
|
Well, for an update. I ended up with 9 layers of 1708 and 1 layer of mat to get about 1/4 to 3/8" which was the same thickness as the wellcraft glass. The transom is 2" thick now.
|
Sounds like it should be plenty.
|